1.2842 Steel for through hardening

Our selected range provides the right material for any application.

Products

Characteristics

Designation

Strength

max. 230 HB
(≈ max. 780 N/mm²)

Chemical composition

Thermal conductivity at 100 °C

33 W/(mK)

Character

Steel for through hardening with very good machinability
High wear resistance and low warping
Good dimensional stability, toughness and through hardenability with uniform hardness for cross sections ≤40 mm

Application

Machining

Unusual:
Polishing, etching, nitriding » 1.2379

Suited:
EDM, hard chrome plating

Use

Cavity plates, mould inserts exposed to abrasive stress, cutting punches
Punch backing plates, die plates and guiding plates, guiding rails

Heat treatment

Soft annealing:
680 to 720 °C, about 2 to 5 hours
Slow, controlled cooling inside the furnace of 10 to 20 °C per hour to about 600 °C
Further cooling in air, max. 220 HB

Hardening:
790 to 820 °C
Quenching in oil/hot bath (200 to 250 °C)
Obtainable hardness: 63−65 HRC

Tempering:
Slow heating to tempering temperature (in order to avoid the formation of cracks) immediately after hardening
Tempering twice with intermediate cooling down to 20 °C increases the toughness
Maximum hardness achievable after tempering: 58–60 HRC

Technical tip

Steel grade 1.2510 is an adequate alternative with regards to its properties, machinability and dimensional stability after heat treatment.

Choix boutique

Construction d’outils de découpe
Construction d’outils de découpe
Construction de machines et de gabarits
Construction de machines et de gabarits

Aperçu du panier

Aperçu CAD

Votre panier est vide.
Montant net
Vers le panier